Barium ferrite tape
Barium ferrite (BaFe) tape is particulate magnetic tape using hexagonal platelet barium ferrite particles instead of metal particles, keeping coercivity at smaller volumes.
Linear tape capacity growth slowed when metal particles reached their size limit. Metal particles are Fe-Co needles whose coercivity comes from shape and drops sharply below about 2,500 nm3, and each needs a passivation layer against oxidation. BaFe is an oxide whose coercivity comes from crystal anisotropy, so it resists oxidation and can be made smaller. [2]
Demonstration particles of 1,600 nm3 reached 223 kA/m coercivity, against 189 kA/m for 2,850 nm3 metal particles, 18% more at 43% less volume. Product particles were 1,950 nm3, and particles of about 1,000 nm3 were also made. After 30 days at 60 °C and 90% relative humidity small metal particles lost much of their magnetization while BaFe was little affected. [2]
The platelets have their easy axis perpendicular to the platelet and can be oriented perpendicular to the tape, with perpendicular squareness of 0.87 on demonstration tape against 0.66 on unoriented product tape. Demonstrations reached 6.7 Gbit/in2 (2006), 29.5 (2010), 85.9 (2014) and 123 Gbit/in2 (2015), equivalent to 8, 35, 154 and 220 TB cartridges, when products held up to 10 TB. [2]
The 123 Gbit/in2 result combined 680 kbit/in with 140 nm tracks read by a 90 nm reader, position error of 5.9 nm or less at 1.23 to 4.08 m/s, and a user bit error rate below 1e-20 after error correction. [3]
Relations
- related
- LTO (Linear Tape-Open), Magnetic tape storage, Metal particle tape, Areal density, Perpendicular magnetic tape, Degaussing
Limitations
Citations
- Oyanagi et al. A High-Density Recording Study on Particulate Magnetic Tape using Barium Ferrite Magnetic Particles. Fujifilm R&D No. 61, 2016.
- Lantz et al. 123 Gbit/in2 Recording Areal Density on Barium Ferrite Tape. IEEE Transactions on Magnetics, November 2015.
Further reading
Sources & caveats
- The main source is a 2016 research paper by the tape-media maker Fujifilm; the 123 Gbit/in2 details come from an IBM Research abstract only.
- Densities are laboratory prototypes with experimental heads and transports; neither source states which LTO generation first used BaFe or gives prices.
- Arithmetic: 25.4 mm / 140 nm is about 181,400 tracks per inch, times 680 kbit/in about 123 Gbit/in2; 223 / 189 = 1.18 and 1,600 / 2,850 = 0.56.